Hey All,

So i just got myself a new abbott and ashby 8" bench grinder, bought along with that a tapered spindle, a stitched buffing pad and a loose buffing pad, some Brown cutting compound for the stitched and some White SS compound for the loose buff.

Fitted it all up and gave it a go for a small 5 minutes or so for each different Buff and compound (one section about 200mm square), stopping to wipe it all clean with Turps before starting on a different compound.

Found the actual side/edge welds came up quickly to a mirror finish but the flats sides of the washer bottle i was doing seems not to be changing much if at all with the use of the compounds and wheels.

my basic Questions are :

1. With brushed alloy material should i be using a sisal buff with a grey compound first to remove the oxidisation from welding then moving down the compound towards to mirror polishing loose buff?

2. Is the grey too harsh and i should spend more time on the brown compound before going to the white?

3. Whats an easy way to tell if more compound is required on the buffing pad?

4. could starting with a 400 or 600 sand paper assist in the polishing process? EDIT : now reading that you can use 400 - 600 - 800 - 1000 grit wet dry prior to final polishing 2nd edit : now reading that using higher than 400 grit is a bad idea - sigh

Any answers and hint would be good.

Cheers

Link to comment
https://www.sau.com.au/forums/topic/177231-aluminium-polishing/
Share on other sites

  • Replies 49
  • Created
  • Last Reply

Top Posters In This Topic

Top Posters In This Topic

Posted Images

Just be carfull when using the compounds that you dont get it too hot, you can easily burn yourself and melt the alloy if you give it some. You can actually get the alloy to "run", although the grinder probably wont have enough grunt to cause too many dramas(ive got 2 of these hooked up together with a bit of 3/4 heater hose for more hp!)

lol....u should stick it on a dyno.

Just thinking of aluminium and bench grinders...whats the best way to tackle a std intake plenum on a 33....pull it off and smash it with a bench grinder?

Craved - You gotta post up some pics when its all done - Did you make it yourself?

Edited by zebra

i polished up my alloy strut brace today. it was originally brushed alluminium. i flattened it out using 320 dry on a sander, then blocked it with 600 wet, then hand rubbed it with 1200 wet. i polished it by hand using meguiers metal polish and it came up like a mirror :)

ill post a pic when i fit it up

  • 3 weeks later...

Worked on my washer bottle with thesand paper and removed most of the marks for the bender. this was working through 4 steps of paper - 400 -600 -800 -1200

then moved onto using the bench grinder and some tripoli on a stitched buff wheel.

then used the white rouge and the loose leaf wheel ... and its was still hazy and not polished :rofl:

Went and bought some meguirs NXT metal polish and wow that stuff works well ... alot more work than using the grinder but really gave more shine on the areas that i did do with the paper then the grinder.

tried it on an area that i didnt sand or use the bench grinder and while it made it shiny it still held residual grain that was present in the alloy.

  • 4 weeks later...

ok mate there is loads of way you can polish and it has been my job for around 3 years kniow the most effective way to polish anything is to get someone else to do it. However if you doooooooneed or want something polished there is a few basic things to consider.

1 onlly alloy and stainless steel should be polished

2 to polish cast mould takes a lot more work.

3 the equiptment i use for all my mirro finsh jobsconsists of...

shinano 6" sander 9000 RPM's

makita barrel grinder with spindel point

120, 240, 500, 600 grit deer round sanding pad ( high rpm rated )

air flow, sizal, loose leaf, swansdown mop ( these are all leaf, stich or rope mops )

fast cut, brown rouge, green chrome ( all cutting compoud bars )

yellow soft compound grease bar and mass finish

That is my basic set up and this will enable the prep and polishing of most stainless and alloy metals

due to some parts haveing tiny hard to reach places sometimes its easier to hand sand and buff on a bench grinders but note there is no way to polish every inch of some things.

cheers for any futher queries about metal polishing, hint or quick tips

i am available after 5 monday to friday and all weekend

cheers kingy

PH 38032143 or 0419771676

Anyone want to polish some pipes for me, or got any good suggestions? They already have a polished finish but they're old. I tried cleaning it with household cleaner (Mr. Muscle etc.) to get the grime off then used normal polish and elbow grease but still looks just as crappy, but slightly cleaner :D.

I’m never polishing anything again, at least nothing as complicated as an RB26 inlet plenum!

I calculated around 40 solid hours to complete, and I didn’t even complete the bottom of it!

- Paint stripped it

- File finished the whole thing, casting marks, letters, deep pits from the sand cast

- Used the above mentioned “fan like” paper sanding drum on the end of a drill, with a small 1” one for between the runners.

- Worked way from 400 600 800 1000 grit. Then went straight to the stitched cotton buffing wheel drill attachment. The finer cutting compound was enough ( I think because I went right up to the 1000 wet and dry)

- Came out really good, I should post some pics up.

I would never ever attempt this again, unless paid an insane amount of money.

Iv heard ppl do a little each night in front of the TV, with it on their lap, but I prefer doing it wet, the paper lasts a lot longer and doesn’t clog.

I’m never polishing anything again, at least nothing as complicated as an RB26 inlet plenum!

I calculated around 40 solid hours to complete, and I didn’t even complete the bottom of it!

- Paint stripped it

- File finished the whole thing, casting marks, letters, deep pits from the sand cast

- Used the above mentioned “fan like” paper sanding drum on the end of a drill, with a small 1” one for between the runners.

- Worked way from 400 600 800 1000 grit. Then went straight to the stitched cotton buffing wheel drill attachment. The finer cutting compound was enough ( I think because I went right up to the 1000 wet and dry)

- Came out really good, I should post some pics up.

I would never ever attempt this again, unless paid an insane amount of money.

Iv heard ppl do a little each night in front of the TV, with it on their lap, but I prefer doing it wet, the paper lasts a lot longer and doesn’t clog.

Get some pics up Michael ;)

Anyone want to polish some pipes for me, or got any good suggestions? They already have a polished finish but they're old. I tried cleaning it with household cleaner (Mr. Muscle etc.) to get the grime off then used normal polish and elbow grease but still looks just as crappy, but slightly cleaner :) .

i would like to mate but its a long way from queensland, try to use a compound called autosol should be able to get it from most auto store. apply compound to surface with finger and work in until all the compound turns black then use a rag in the same motion this will remove most of the residue finally use a clean rag over the surface again and this will remove remaining compound.

this is a cheap fix and will not take out any deep scores or scratches but will improve the shine of the part.

CRAVED: so how do you know when more compound is required on the buffing wheel?

with a course compound I.E. fast cut ( grey ) brown rouge ( brown ) apply till mop is completely coated on parant surface. the best way to tell is when you are barrelling ( polishing ) pull the job against the direction of mop this will apply the compound to the job and after this run over the same spot this will rooll over the metal and help with a better shine. applying cutting compound is simple on your backward stroke if very little or no compound is released from mop then it is time to reapply.

However with a green chrome compound less is more the more you put on the mop the more you have to get off allt he green is for is to take of the brown or grey coating giving you the mirror finish you want.

( P.S. in my expierience the white compound is to fine for metal and i only use it to polish plastics. but i do have acces to the green chrome. so if it works go with it. )

Create an account or sign in to comment

You need to be a member in order to leave a comment

Create an account

Sign up for a new account in our community. It's easy!

Register a new account

Sign in

Already have an account? Sign in here.

Sign In Now



  • Similar Content

  • Latest Posts

    • Hi, SteveL Thank you very much for your reply, you seem to be the only person on the net who has come up with a definitive answer for which I am grateful. The "Leak" was more by way of wet bubbles when the pedal was depressed hard by a buddy while trying to gey a decent pedal when bleeding the system having fitted the rebuilt BM50 back in the car, which now makes perfect sense. A bit of a shame having just rebuilt my BM50, I did not touch the proportioning valve side of things, the BM50 was leaking from the primary piston seal and fluid was running down the the Brake booster hence the need to rebuild, I had never noticed any fluid leaking from that hole previously it only started when I refitted it to the car. The brake lines in the photo are "Kunifer" which is a Copper/Nickel alloy brake pipe, but are only the ones I use to bench bleed Master cylinders, they are perfectly legal to use on vehicles here in the UK, however the lines on the car are PVF coated steel. Thanks again for clearing this up for me, a purchase of a new BMC appears to be on the cards, I have been looking at various options in case my BM50 was not repairable and have looked at the HFM BM57 which I understand is manufactured in Australia.  
    • Well the install is officially done. Filled with fluid and bled it today, but didn't get a chance to take it on a test drive. I'll throw some final pics of the lines and whatnot but you can definitely install a DMAX rack in an R33 with pretty minor mods. I think the only other thing I had to do that isn't documented here is grind a bit of the larger banjo fitting to get it to clear since the banjos are grouped much tighter on the DMAX rack. Also the dust boots from a R33 do not fit either fyi, so if you end up doing this install for whatever reason you'll need to grab those too. One caveat with buying the S15 dust boots however is that the clamps are too small to fit on the R33 inner tie rod since they're much thicker so keep the old clamps around. The boots also twist a bit when adjusting toe but it's not a big deal. No issues or leaks so far, steering feels good and it looks like there's a bit more lock now than I had before. Getting an alignment on Saturday so I'll see how it feels then but seems like it'll be good to go       
    • I don't get in here much anymore but I can help you with this.   The hole is a vent (air relief) for the brake proportioning valve, which is built into the master cylinder.    The bad news is that if brake fluid is leaking from that hole then it's getting past the proportioning valve seals.   The really bad news is that no spare parts are available for the proportioning valve either from Nissan or after market.     It's a bit of a PITA getting the proportioning valve out of the master cylinder body anyway but, fortunately, leaks from that area are rare in my experience. BTW, if those are copper (as such) brake lines you should get rid of them.    Bundy (steel) tube is a far better choice (and legal  in Australia - if that's where you are).
×
×